    Equipment Required for Blasting work -
    1. Air compressor with Moisture separator.
    2. Copper Slag/ Sand Blasting with hose pipe connected Nozzle.
    3. LPG Burner, Hose pipe and LPG Cylinders.
    Measuring and Test Equipments :-
    1. Peel Gauge Tester. (Weight Balance for weight check while removing of peel)
    2. Pyrometer/ Infrared Temp. Gun. (For Measuring temp of pipe surface)
    3. Holiday Detector. (For Coating Damage Check)
    4. Hygrometer(For Relative Humidity Check)
    5. Coat meter / Elcometer (For Coating Sleeve Thickness Measurement)
    6. Wet film thickness gauge (For Primer Thickness Measurement)
    7. Roughness profile measuring (Styled) instrument. (For Surface Roughness Comparison)
    8. Press O Film (Thickness 50µm for roughness impression on it)
    9. Digital Micrometer (For Roughness measurement printed on Press-O-Film)
    Note - All measuring and test Equipment shall be calibrated.
    This video contain all step follow during Field Joint Coating of Pipeline :
    1.Chamfering of 3LPE Coating at angle 30° with horizontal, 3LPE coating from Factory was chamfered at site.
    2. Checking of Relative Humidity with Hygrometer. As per standard relative humidity is less than 85 %.
    3. Blasting of Welded exposed Metal surface with Nozzle and sweep blast- 100 mm sleeve
    overlap area on 3LPE mill coating.
    4. After Blasting check for surface roughness with Press-O-Film which is 50-70 micron as per standard specification..
    5. Dust Contamination check with Tape (As per ISO-8502-3) maximum allow rating is 2.
    6. Pre-heat the surface before applying the epoxy primer. Pre-heat Temperature 60-70 ℃.
    7. application of Epoxy Primer
    Mixed epoxy primer Part A : Part B in ration of 3:1 mixing duration is 30-60 Sec.
    Primer application only on steel surface.
    8. check the primer thickness with the Wet Film Thickness Gauge. Primer thickness is greater than 200 microns.
    9.Apply HTLP-80 sleeve on wet primer in Centre of weld joint. Sleeve overlap is at 10 or 2 O'clock.
    10. Application of Closure Patch with inner preheating and apply roller by pressing over it or all over the surface of sleeve.
    11. Holiday test at 15 kv for 12.75 inch pipe Diameter.
    Visual Inspection :
    * Adhesive flow evident over the entire circumference on both edges.
    * Coating Sleeve free from Air Entrapments & Air Voids.
    * Sleeve Surface free from Bums & Punctures.
    cgd
    pipe coating
    gas pipe line
    hdpe welding
    pqr
    Seal For Life HSS Field Presentation at Selam CGD Project
    Testing the adhesion of a pipeline coating also know as "Peel Test"
    How to avoid corrosion in underground-pipes by applying PVC-bitumen tapes
    3 Layer Polyethylene Coating (3LPE) - Pipe Coating
    Heat shrinkable sleeve for steel pipes
    FRDP Dry Film Heat Shrink Sleeve Installation Guide
    Heat Shrinkable wrap sleeves for Pipeline
    3LPE Coating Pipe Process
    How to avoid corrosion in underground-pipes by applying PVC-bitumen tapes
    Pipeline Coating damage repair | Patch repair I 3LPE Coating
    Pipeline Coating damage repair | Patch repair I 3LPE Coating
    Joint coating of 12" 3LPE Product Pipeline (IOCL PAJPL-Una Branch Product Pipeline) (PB to HP, IN)
  • Наука та технологія

КОМЕНТАРІ • 29