  • How to screen printing HD glossy silicone on mesh shoe upper? Preparation:
    1.Mesh&Squeegee: 120(48T) Mesh number ;65-75 degree Squeegee.
    2.Pigments added ratio:For white and fluorescent color 20%,other color 10%
    3.Catalyst mixing ratio:10% slow dry XG-MB-1 Extra slow dry catalyst XG-TMB-1
    4.Silicone thinner XG-128AH adding ratio:0-20%
    5.Heating Temp :60℃~100℃
    Printing process:
    Step1:PU based for under printing for 6 layers to get smooth layer first
    HD PU water based nylon Ink XGS-806 100 G
    Fixer XGS-339 2G 2% Flash by 80℃- 100℃.
    Have to make sure to get PU based 100% dry and clear first,then move to print silicone crossing linker and silicone ink or will lead crossing linker and silicone ink not easy to dry and layers peal off from PU based ink .
    Step2:Silicone crossing linker for mid layer printing for 2 layers:
    Silicone crossing linker XG-360Z-3X 50G
    Silicone catalyst XG-866B-2+ 4G
    Flash by 100-120 ℃
    Step3:Silicone High density printing 4-6 layer
    Screen Printing Silicone XG-866A-2Y 100G
    Silicone fast dry catalyst XG-866B-2 3G
    Silicone thinner XG-128AH 10G
    Flash by 100℃- 120℃
    Step4: Color effect silicone printing for 4-6 layers:
    For bright color pigment and white color mixing to print for 2-3 layers
    Screen Printing Silicone XG-866A-2Y 100G
    White silicone pigment XG-102 5G
    Color silicone pigment XG-series 5G
    Silicone fast dry catalyst XG-866B-2 3G
    Silicone thinner XG-128AH 10G
    This step if for bright color effect printing to get good printing effect and coverage.
    Step5: Color silicone layer print 3 layers
    Screen Printing Silicone XG-866A-2Y 100G
    Color silicone pigment XG-series 20G
    Silicone fast dry catalyst XG-866B-2 3G
    Silicone thinner XG-128AH 10G
    Flash by 100℃- 120℃
    Step6.Glossy silicone ink for top coating printing 2 layers
    Glossy silicone XG-399-3 100 G
    Silicone fast dry catalyst XG-866B-2 3G
    Silicone thinner XG-128AH 10G
    To get silicone bubbles out first ,try to use cold wind to support and it will be better to use low temp by longer heating time to avoid bubbles problem.
    Cure by 60℃~80℃
    For more silicone ink information kindly follow our website :www.xgsilicone.com or contact with Lily :+86 13825488489 whatsapp&wechat the same number