    Preparation:
    1.Mesh&Squeegee:Mesh number 120(48T) for under printing color,300-300(80-120T)for CMYK color printing ;65-75 degree Squeegee.
    2.: Pigments added ratio:For CMYK effect Color mixing ratio 20%
    3.Catalyst mixing ratio:2% slow dry XG-866B-1 and fast dry XG-866B-2 can mix together for using.
    4.Silicone thinner XG-128AH adding ratio:20% Silicone thinner is necessary for CMYK printing
    5.Heating Temp and time: Flash cure temp :130℃ for 6-10 seconds ,Drying temp :120℃- 140℃ for about 2 -3 minutes.
    Process:
    Step1:.Under print color effect print 1 layer, CMYK color print 2 layers :
    Elastic soft silicone XG-866NYR+ 100G
    Color pigment XG- color 20G 20%
    Fast dry catalyst XG-866B-2 2G 2% If machine printing to use slow dry catalyst.
    Silicone thinner XG-128AH 20G 20%
    Cure by temp of 130℃ 6-10 seconds.
    Step2.Matte top coating for 2 layers:
    Matte silicone XG-866M-6+ 50G
    Fast dry catalyst XG-866B-2 1G 2% If machine printing to use slow dry catalyst.
    Silicone thinner XG-128AH Silicone thinner is not necessary for matte silicone.
    Cure by temp of 120℃ 6-10 seconds.
    After printing finish, to heat by 120℃- 140℃ for about 2 -3 minutes.
    For more silicone ink information kindly follow our website :www.xgsilicone.com or contact with Lily :+86 13825488489 whatsapp&wechat the same number